How to Print XG HD glossy silicone for horse riding pants printing?

How to Print XG HD glossy silicone for horse riding pants printing?

Preparation:

  • Mesh&Squeegee: 120(48T) Mesh number ;65-75 degree Squeegee.
  • : Pigments added ratio:For white and fluorescent color 20%,other color 10%
  • Catalyst mixing ratio:2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for using.
  • Silicone thinner XG-128A adding ratio:0-20%    Silicone thinner is not necessary for hand printing
  • Heating Temp and time: cure temp :100℃- 120℃ for 6-10 seconds ,Drying temp :120℃- 140℃ for about 2 -3 minutes.

Silicone ink printing tips:

1. Under coating silicone XG-136A-1/XG-136B-1 for under coating printing for 2 times :

Under coating  silicone         XG-136A-1        50G

Under coating  silicone         XG-136B-1        50G

XG-136A-1: XG-136B-1 mixing ratio 50%:50%.

Cure by temp of 120℃ 6-10 seconds.

If for machine printing to use XG-136A&XG-136B same mixing ratio.

2A. Color effect silicone printing for 3 times : 

HD silicone           XG-866AH        50G

White color pigment    XG-102          10G For white and fluorescent color 20%,other color 10%

Fast dry catalyst       XG-866B-2       1G  2%  If machine printing to use slow dry catalyst.

Silicone thinner     XG-128AH Silicone thinner is not necessary for hand printing,10% for machine printing. Cure by temp of 120℃ 6-10 seconds.

2B. Transparent round silicone XG-866A-2Y printing for 3 times

Round silicone           XG-866A-2y        50G

Silicone thinner          XG-128AH          10G   20%

Fast dry catalyst       XG-866B-2       1G  2%  this code can not work on machine. 

Flash by temp of 120℃ 6-10 seconds.

3. Glossy silicone ink silicone ink for top coating:

 Glossy top coating for 2 times:

Glossy silicone ink   XG-399-3  50G

Fast dry catalyst  XG-866B-2      1G  2%  It will be better to use slow dry catalyst XG-866B-1 and fast dry half and half. If for machine printing to use slow dry catalyst.

Silicone thinner     XG-128AH  Silicone thinner is not necessary for hand printing,5-10% is enough for machine printing.  Have to get silicone bubbles out first ,try to use code wind to support and it will be better to use low temp by longer heating time to avoid bubbles problem.

Flash by temp of 120℃ 6-10 seconds.

After printing finish, to heat by 120℃- 140℃ for about 2 -3 minutes.

HD glossy silicone for horse riding pants printing
HD glossy silicone for horse riding pants printing
HD glossy silicone for horse riding pants printing

[video_embed url=”http://www.youtube.com/watch?v=4WuOEf2sjew”] [space_box id=”” height=”10″]

[video_embed url=”http://www.youtube.com/watch?v=eFqPh0v-96Q”] [space_box id=”” height=”10″]