Silicone Pulling Stone Printing

Silicone Pulling Stone Printing

XG silicone HD pulling stone printing ,3D mountain effect printing

Silicone pulling stone printing,machine printing silicone printing

Preparation:

Mesh&Squeegee: 120(48T) Mesh number ;65-75 degree Squeegee.

: Pigments added ratio:For white and fluorescent color 20%,other color 10%

Catalyst mixing ratio:2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for using.

Thinner XG-128A adding ratio:10-30% thinner is very necessary for pulling stone printingHeating Temp and time: Flash cure temp :100℃- 120℃ for 6-10 seconds ,Drying temp :120℃- 140℃ for about 2 -5 minutes.

Printing process :

1st HD silicone under coating for two times      

HD silicone XG-866AH/866A      300G

Fast dry catalyst XG-866B-2    6G    2%

Thinner  XG-128AH              30G   10%

HD clear to print for two times Heating temp 120-140degree

2nd HD color effect printing

HD silicone XG-866AH/866A      300G

Fast dry catalyst XG-866B-2    6G    2%

Color pigment  30G 10-20%(white and fluorescent color 20%)

Thinner XG-128AH 30G 10%HD color to print 2 times

Flash temp 120-140degree

3rd Pulling printing

HD silicone XG-866AH/866A      300G

Round silicone XG-866A-2Y      300G

Fast dry catalyst XG-866B-2    12G    2%

Color pigment  60G 10-20%(white&fluorescent color 20%)

Thinner XG-128AH 180G 30%Heating temp 120-140degree for 2-3 minutes

Key point for pulling pirnting

1,Silicone mix with 20-30% thinner

2,The angel between squeegee & table 60-70 degree

3.Keep distance between printing squeegee & screen

4,Less pressure print very soft and slowly5,Move up screen slowly

XG silicone pulling stone HD printing effect
XG silicone pulling stone printing effect
XG silicone pulling stone HD printing effect