Silicone CMYK Color Screen Printing

Silicone-CMYK-printing-CMYK-silicoe-ink-printing

Silicone CMYK Color Screen Printing

Tag: Silicone CMYK printing, silicone color printing, CMYK printing, silicone screen printing

Preparation:

  1. Mesh&Squeegee: 300(120T) Mesh number ;70-75 degree Squeegee.
  2. : Pigments added ratio:10-20%
  3. Catalyst mixing ratio:2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for using.
  4. Thinner XG-128AH adding ratio:20%    
  5. Heating Temp and time: Flash cure temp :120℃- 140for 6-10 seconds ,Drying temp :120℃- 140for about 2-3  minutes.

Silicone ink printing tips:

HD silicone     XG-866A/866AH        100G

Color pigment                          15G   15%

Fast dry catalyst   XG-866B-2           2G  2%   If machine printing to use slow dry catalyst.

Thinner     XG-128AH                  20G  20%

Flash by temp of 120℃ for 6-10 seconds.

If dark color fabric print CMYK effect need to print a full screen printing white color for 1-2 times first then print CMYK effect.

If fabric with hairy have to print a full screen printing for under printing two times ,for first time printing  assist by heat press machine or iron after first time printing to get good smooth. After printing keep wet to heat press by temp 150-170 degree for 10-20 seconds.Second printing same as normal silicone printing heat by 120℃- 140℃ for 6-10 seconds.

After finish to heat by heating tunnel by 120-140 degree for 2 -3 minutes

silicone CMYK ink printing Silicone CMYK printing
Silicone CMYK printing CMYK silicone ink printing
silicone-ink-CMYK-screen-printing
Silicone-ink-CMYK-screen-printing

Silicone CMYK printing video: