How to print silicone for under wear bonding?
Silicone printing tips for underwear bonding printing
Preparation:
1.60-80(24-32T) 65-75 degree Squeegee.
2.Catalyst mixing ratio:3%
3.Silicone thinner XG-128A adding ratio:20-30% Heating Temp and time: Flash cure temp: 120℃ for 6-10 seconds ,Drying temp: 100℃for about 10 minutes.
Screen printing silicone ink for underwear bonding printing:
1.Underwear bonding silicone ink print 5 layers:
Underwear bonding silicone XG-866NY-2 100G
Silicone thinner XG-128AH 20-30G 20-30%
Fast dry catalyst XG-866B-2 3G 3%
Cure by temp of 100-120℃ 8-12 seconds.
2.To print Underwear bonding silicone ink wet on wet two layers.
The same mixing ratio as above.
3.To stick a piece of underwear fabric on printed fabric, and smooth by empty printing
4.Cure by 100-120℃ 8-12 seconds.
5.Embossing heat press by 180 degree for 20 seconds
6.Cure by 100 degree for 10 minutes