Firstly, to print under printing,

Second, to print white silicone,

Third, to print colorful silicone,

Fourth, to print chameleon powder with printing silicone ink,

In the end, to print glossy silicone ink.

For the printing process kindly follow the below tips.

Screen printing silicone ink preparation and screen printing silicone mixing ratio:

1.Mesh & Squeegee for Screen Printing Silicone Ink:

120(48T) Mesh number;

65-75 degree Squeegee.

2.Pigments added ratio for Screen Printing Silicone Ink:

For white and fluorescent colors 20%, other colors 10%,

chameleon powder mixing ratio10%.

3.Screen Printing Silicone Ink Catalyst mixing ratio:

2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for use.

4. Screen Printing Silicone Ink thinner XG-128A adding ratio: 0-20%   

Notes: Silicone thinner is not necessary for hand printing

5.Screen Printing Silicone Ink Heating Temp and time: Flash cure temp for Screen Printing Silicone Ink :100℃- 120℃ for 6-10 seconds, Drying temp :120℃ for about 2 minutes.

Printing process:

1st.HD silicone for under printing 1 layer:

HD silicone          XG-866A    100G

Silicone catalyst   XG-866B-2      2G  2%

Heating temp 120 Degree

2nd.White silicone print 2 layers:

HD silicone          XG-866A  100G

White pigment        XG-102   20G  20%

Silicone catalyst   XG-866B-2   2G  2%

Heating temp 120 Degree

3rd.Color silicone print 2 layers:

HD silicone          XG-866A  100G

White pigment        XG-102   20G  20%

Silicone catalyst   XG-866B-2   2G  2%

Heating temp 120 Degree

4th.Screen printing silicone chameleon powder print 2 layers:

Screen printing silicone   XG-866A-2Y  100G

Chameleon powder                   10G  10%

Silicone thinner          XG-128AH  10-20G  10-20%

Silicone catalyst           XG-866B-2  2G  2%

Heating temp 120 Degree

5th.Glossy silicone for top coating 1-2 layers:

Glossy silicone ink   XG-399-3    100G

Fast dry catalyst  XG-866B-2      2G  2%

Heating temp 100-120 Degree Have to get silicone bubbles out first, try to use code wind to support and it will be better to use low temp by longer heating time. To avoid bubbles problem.

Chameleon Silicone Printing HD glossy silicone Screen Printing Silicone
HD Glossy Screen Printing Silicone Chameleon Silicone Printing

Share this post

0 0 votes
Article Rating
Subscribe
Notify of
guest
0 评论
Inline Feedbacks
View all comments

Hello~

0
Would love your thoughts, please comment.x
()
x