HD Matte Silicone Effect Print on Waterproof Fabric
Preparation:
- Mesh&Squeegee: 120(48T) Mesh number ;65-75 degree Squeegee.
- : Pigments added ratio:For white and fluorescent color 20%,other color 10%
- Catalyst mixing ratio:2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for using.
- Thinner XG-128A adding ratio:0-20% thinner is not necessary for hand printing
- Heating Temp and time: Flash cure temp :20℃ for 6-10 seconds ,Drying After printing finish, to heat by 100℃ for -20 minutes to get crossing linker with excellent fastness on special coating water proof fabric.
Printing tips:
1.Crossing liner for under coating for 2 times
Crossing linker XG-360Z-3 20G
Crossing linker agent XG-360Z-3B 1G 5%
2.HD silicone for high density print for 2-4 times
HD silicone XG-866AH 50G
Catalyst XG-866B-2 1G 2%
Thinner XG-128AH thinner is not necessary,to mix 10% can get easy print.
Heating temp: 120 degree
3.White HD silicone for 4 times
HD silicone XG-866AH 50G
White pigments XG-102 10G
Catalyst XG-866B-2 1G 2%
Thinner XG-128AH thinner is not necessary,to mix 10% can get easy print.
Heating temp: 120 degree
4.Matte silicone for top coating for 1 time
Matte silicone XG-866M 30G
Catalyst XG-866B-2 0.6G 2%
Thinner XG-128AH thinner is not necessary,to mix 10% can get easy print.
Heating temp: 120 degree
After printing finish, to heat by 100℃ for 20 minutes to get crossing linker with excellent fastness on special coating water proof fabric.